耐候结构钢的力学性能和工艺性能(GB/T 4171—2008) |
||||||||||||
|
牌号 |
拉伸试验① |
180°弯曲试验 弯心直径 |
||||||||||
|
下屈服强度ReL/(N/mm2) 不小于 |
抗拉强度 Rm/(N/mm2) |
断后伸长率A/% 不小于 |
||||||||||
|
≤16 |
>16~ 40 |
>40~ 60 |
>60 |
≤16 |
>16~ 40 |
>40~ 60 |
>60 |
≤16 |
>6~ 16 |
>16 |
||
|
Q235NH |
235 |
225 |
215 |
215 |
360~510 |
25 |
25 |
24 |
23 |
a |
a |
2a |
|
Q295NH |
295 |
285 |
275 |
255 |
430~560 |
24 |
24 |
23 |
22 |
a |
2a |
3a |
|
Q295GNH |
295 |
285 |
— |
— |
430~560 |
24 |
24 |
— |
— |
a |
2a |
3a |
|
Q355NH |
355 |
345 |
335 |
325 |
490~630 |
22 |
22 |
21 |
20 |
a |
2a |
3a |
|
Q355GNH |
355 |
345 |
— |
— |
490~630 |
22 |
22 |
— |
— |
a |
2a |
3a |
|
Q415NH |
415 |
405 |
395 |
— |
520~680 |
22 |
22 |
20 |
— |
a |
2a |
3a |
|
Q460NH |
460 |
450 |
440 |
— |
570~730 |
20 |
20 |
19 |
— |
a |
2a |
3a |
|
Q500NH |
500 |
490 |
480 |
— |
600~760 |
18 |
16 |
15 |
— |
a |
2a |
3a |
|
Q550NH |
550 |
540 |
530 |
— |
620~780 |
16 |
16 |
15 |
— |
a |
2a |
3a |
|
Q265GNH |
265 |
— |
— |
— |
≥410 |
27 |
— |
— |
— |
a |
— |
— |
|
Q310GNH |
310 |
— |
— |
— |
≥450 |
26 |
— |
— |
— |
a |
— |
— |
|
注:a为钢材厚度。 ① 当屈服现象不明显时,可以采用Rp0.2。 |
||||||||||||